{"id":8721,"date":"2025-05-21T14:29:11","date_gmt":"2025-05-21T14:29:11","guid":{"rendered":"https:\/\/premiumalu.com\/6013-aluminum-everything-you-need-to-know\/"},"modified":"2026-10-05T14:10:35","modified_gmt":"2026-10-05T14:10:35","slug":"6013-aluminio-tudo-o-que-voce-precisa-saber","status":"publish","type":"post","link":"https:\/\/premiumalu.com\/pt\/6013-aluminum-everything-you-need-to-know\/","title":{"rendered":"Tudo o que voc\u00ea precisa saber sobre o alum\u00ednio 6013"},"content":{"rendered":"<p class=\"wp-block-paragraph\">O 6013 existe para um problema de projeto: uma pe\u00e7a que precisa de resist\u00eancia da classe 2024-T3, mas tem de ser soldada. O 6061 solda, mas esgota a sua resist\u00eancia logo acima de 310 MPa em T6. O 2024-T3 tem a resist\u00eancia, mas n\u00e3o \u00e9 uma liga de soldadura por fus\u00e3o e necessita de revestimento ou pintura para sobreviver em servi\u00e7o.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O 6013 resolve esse problema pelo lado da s\u00e9rie 6xxx. \u00c9 uma liga Al-Mg-Si-Cu trat\u00e1vel termicamente, com limite de escoamento em T6, tenacidade \u00e0 fratura e comportamento \u00e0 fadiga pr\u00f3ximos dos da chapa 2024-T3, soldando como um grau 6xxx e n\u00e3o necessitando de revestimento protetor.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Dois limites, ent\u00e3o, decidem a especifica\u00e7\u00e3o. O cobre que torna o 6013 mais resistente que o 6061 tamb\u00e9m aumenta a sua tend\u00eancia \u00e0 corros\u00e3o intergranular, e a resist\u00eancia m\u00e1xima s\u00f3 \u00e9 atingida ap\u00f3s uma etapa de tratamento t\u00e9rmico que tem de ser inclu\u00edda no roteiro de processo.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img fetchpriority=\"high\" decoding=\"async\" width=\"800\" height=\"600\" src=\"https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-Aluminum-Guide.png\" alt=\"\" class=\"wp-image-10624\" srcset=\"https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-Aluminum-Guide.png 800w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-Aluminum-Guide-300x225.png 300w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-Aluminum-Guide-768x576.png 768w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-Aluminum-Guide-16x12.png 16w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-Aluminum-Guide-600x450.png 600w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">O que \u00e9 o alum\u00ednio 6013?<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A resist\u00eancia nesta liga vem do endurecimento por precipita\u00e7\u00e3o, e n\u00e3o do trabalho a frio. O magn\u00e9sio e o sil\u00edcio combinam-se em Mg\u2082Si, e a adi\u00e7\u00e3o de cobre promove fases adicionais contendo Cu que elevam tanto a resist\u00eancia como a resist\u00eancia \u00e0 fadiga acima do que uma liga Al-Mg-Si simples alcan\u00e7a.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\u00c9 uma adi\u00e7\u00e3o relativamente recente \u00e0 fam\u00edlia 6xxx e continua a ser um grau de nicho. N\u00e3o o encontrar\u00e1 em stock t\u00e3o amplamente como o 6061, e o pr\u00e9mio sobre o 6061 \u00e9 real. Os compradores especificam-no por duas raz\u00f5es: precisam de mais resist\u00eancia que o 6061 numa liga sold\u00e1vel, ou precisam de propriedades da classe 2024-T3 numa pe\u00e7a que tem de ser soldada ou que n\u00e3o pode tolerar o comportamento \u00e0 corros\u00e3o do 2024.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Composi\u00e7\u00e3o qu\u00edmica<\/h2>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td>Elemento<\/td><td>Intervalo (% em peso)<\/td><\/tr><tr><td>Sil\u00edcio (Si)<\/td><td>0.60 \u2013 1.0<\/td><\/tr><tr><td>Magn\u00e9sio (Mg)<\/td><td>0.80 \u2013 1.2<\/td><\/tr><tr><td>Cobre (Cu)<\/td><td>0.60 \u2013 1.1<\/td><\/tr><tr><td>Mangan\u00eas (Mn)<\/td><td>0.20 \u2013 0.80<\/td><\/tr><tr><td>Ferro (Fe)<\/td><td>\u2264 0,50<\/td><\/tr><tr><td>Zinco (Zn)<\/td><td>\u2264 0.25<\/td><\/tr><tr><td>Cromo (Cr)<\/td><td>\u2264 0,10<\/td><\/tr><tr><td>Tit\u00e2nio (Ti)<\/td><td>\u2264 0,10<\/td><\/tr><tr><td>Outros (cada \/ total)<\/td><td>\u2264 0,05 \/ \u2264 0,15<\/td><\/tr><tr><td>Alum\u00ednio (Al)<\/td><td>Restante (94,8 \u2013 97,8)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Dois pontos importam mais do que os pr\u00f3prios n\u00fameros. O sil\u00edcio e o magn\u00e9sio encontram-se numa propor\u00e7\u00e3o quase equilibrada para a forma\u00e7\u00e3o de Mg\u2082Si, que \u00e9 o que torna a liga suscet\u00edvel ao envelhecimento artificial.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O teor de cobre \u00e9 o outro ponto. A at\u00e9 1,1% \u00e9 aproximadamente tr\u00eas a cinco vezes o que o 6061 permite, o que explica tanto por que o 6013 \u00e9 mais resistente que o 6061 como por que \u00e9 menos tolerante \u00e0 corros\u00e3o.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Especifica\u00e7\u00f5es e Designa\u00e7\u00f5es Equivalentes<\/h2>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td>Sistema<\/td><td>Designa\u00e7\u00e3o<\/td><\/tr><tr><td>UNS<\/td><td>A96013<\/td><\/tr><tr><td>ISO<\/td><td>AlMg1Si0.8CuMn<\/td><\/tr><tr><td>ASTM<\/td><td>B209 (chapa e placa), B221 (barra extrudida, vergalh\u00e3o, tubo, perfis)<\/td><\/tr><tr><td>AMS<\/td><td>4216 (chapa 6013-T6), 4347 (chapa 6013-T4)<\/td><\/tr><tr><td>GB\/T<\/td><td>3190<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Ao redigir a ordem de compra, indique a especifica\u00e7\u00e3o e o temper juntamente. \u201c6013\u201d por si s\u00f3 n\u00e3o define um n\u00edvel de resist\u00eancia \u2014 6013-T4 e 6013-T6 diferem em cerca de 100 MPa no limite de escoamento, o que \u00e9 a diferen\u00e7a entre uma pe\u00e7a que aguenta e uma que n\u00e3o aguenta.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Propriedades Mec\u00e2nicas por T\u00eampera<\/h2>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td>Temperamento<\/td><td>Resist\u00eancia \u00e0 tra\u00e7\u00e3o (MPa)<\/td><td>Limite de escoamento (MPa)<\/td><td>Alongamento<\/td><td>Resist\u00eancia \u00e0 fadiga (MPa)<\/td><td>Resist\u00eancia ao corte (MPa)<\/td><td>Dureza (HB)<\/td><\/tr><tr><td>T4<\/td><td>~310<\/td><td>~170<\/td><td>~22%<\/td><td>~98<\/td><td>~190<\/td><td>\u2014<\/td><\/tr><tr><td>T6<\/td><td>379 \u2013 410<\/td><td>~350<\/td><td>~9%<\/td><td>~140<\/td><td>~240<\/td><td>~130<\/td><\/tr><tr><td>T651<\/td><td>\u2265 379<\/td><td>\u2265 359<\/td><td>\u2265 5%<\/td><td>~110<\/td><td>240 \u2013 248<\/td><td>130<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">A linha T651 \u00e9 extra\u00edda dos valores m\u00ednimos dos produtores de alum\u00ednio para placa; a chapa T6 tipicamente ensaia para o extremo superior da sua banda. Trate a tabela como uma ferramenta de triagem e o certificado de ensaio da f\u00e1brica como o documento vinculativo \u2014 os m\u00ednimos garantidos variam com a espessura e a forma do produto.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Vale a pena notar: o T6 tem a maior resist\u00eancia \u00e0 fadiga dos tr\u00eas tempers, cerca de 140 MPa, enquanto o T651 fica mais baixo, a aproximadamente 110 MPa, apesar de uma resist\u00eancia est\u00e1tica marginalmente superior. Se a pe\u00e7a \u00e9 limitada por fadiga e n\u00e3o por est\u00e1tica, essa diferen\u00e7a deve determinar a escolha do temper, e n\u00e3o o valor do limite de escoamento.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Propriedades f\u00edsicas<\/h2>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td>Propriedade<\/td><td>Valor<\/td><\/tr><tr><td>Densidade<\/td><td>2,71 \u2013 2,72 g\/cm\u00b3<\/td><\/tr><tr><td>Faixa de fus\u00e3o<\/td><td>~579 \u2013 650 \u00b0C<\/td><\/tr><tr><td>Condutividade t\u00e9rmica<\/td><td>~150 \u2013 164 W\/m\u00b7K<\/td><\/tr><tr><td>Condutividade el\u00e9trica<\/td><td>~35% IACS<\/td><\/tr><tr><td>Coeficiente de expans\u00e3o t\u00e9rmica<\/td><td>23,4 \u00d7 10\u207b\u2076 \/\u00b0C (20 \u2013 100 \u00b0C)<\/td><\/tr><tr><td>M\u00f3dulo de elasticidade<\/td><td>69 \u2013 71 GPa<\/td><\/tr><tr><td>Temperatura m\u00e1xima de servi\u00e7o<\/td><td>~160 \u00b0C<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">A condutividade el\u00e9trica \u00e9 o valor mais frequentemente citado incorretamente. Devido ao teor de cobre, o 6013 situa-se perto de 35% IACS \u2014 abaixo do 6061, n\u00e3o acima. Qualquer aplica\u00e7\u00e3o que dependa da condutividade em vez da resist\u00eancia deveria considerar o 6061, o 6063 ou o 6101.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Tempers: T4, T6 e T651<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>T4<\/strong> \u00e9 submetido a tratamento t\u00e9rmico de solubiliza\u00e7\u00e3o e envelhecido naturalmente. \u00c9 o mais macio dos tr\u00eas e aquele em que se conforma \u2014 a conformabilidade em T4 \u00e9 reportada como amplamente compar\u00e1vel \u00e0 do 2024-O. O alongamento situa-se em torno de 22%, o que permite curvas apertadas e estampagens profundas.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>T6<\/strong> \u00e9 submetido a tratamento t\u00e9rmico de solubiliza\u00e7\u00e3o e envelhecido artificialmente at\u00e9 \u00e0 resist\u00eancia m\u00e1xima. Esta \u00e9 a condi\u00e7\u00e3o de entrega para a maioria das pe\u00e7as estruturais e para chapa.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>T651<\/strong> \u00e9 T6 com uma etapa adicional de al\u00edvio de tens\u00f5es \u2014 o material \u00e9 estirado numa quantidade controlada antes do envelhecimento artificial. O estiramento \u00e9 o que melhora a estabilidade dimensional durante e ap\u00f3s a maquinagem, pelo que o T651 \u00e9 a designa\u00e7\u00e3o para placa que ser\u00e1 fortemente fresada. A chapa \u00e9 normalmente fornecida como T6 e n\u00e3o como T651, porque a etapa de estiramento \u00e9 uma opera\u00e7\u00e3o de placa e barra.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">A rota de conformar e depois envelhecer<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Esta \u00e9 a raz\u00e3o pela qual muitas oficinas especificam o 6013, e \u00e9 o ponto que a maioria das fichas t\u00e9cnicas omite. O envelhecimento natural em T4 prossegue lentamente, pelo que uma pe\u00e7a pode ser conformada em T4 e depois envelhecida diretamente at\u00e9 \u00e0 resist\u00eancia m\u00e1xima em T6 <strong>sem um segundo tratamento t\u00e9rmico de solubiliza\u00e7\u00e3o<\/strong>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Para compara\u00e7\u00e3o, o 2024-W tem de ser refrigerado para manter a sua conformabilidade, e a maioria das pe\u00e7as 6xxx que s\u00e3o conformadas e depois envelhecidas necessitam primeiro de um novo tratamento de solubiliza\u00e7\u00e3o. Saltar essa re-t\u00eampera no 6013 significa menos distor\u00e7\u00e3o a corrigir, menos etapas de processo e nenhum recontrolo da estrutura de gr\u00e3o. Se a sua pe\u00e7a \u00e9 grande, fina ou sens\u00edvel \u00e0 distor\u00e7\u00e3o, s\u00f3 esta rota pode justificar o pr\u00e9mio da liga.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Trabalhar com o 6013<\/h2>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" width=\"800\" height=\"600\" src=\"https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Working-With-6013-Corrosion-Limits.png\" alt=\"\" class=\"wp-image-10627\" srcset=\"https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Working-With-6013-Corrosion-Limits.png 800w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Working-With-6013-Corrosion-Limits-300x225.png 300w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Working-With-6013-Corrosion-Limits-768x576.png 768w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Working-With-6013-Corrosion-Limits-16x12.png 16w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Working-With-6013-Corrosion-Limits-600x450.png 600w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">Conforma\u00e7\u00e3o<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Fa\u00e7a a conforma\u00e7\u00e3o em T4. Em T6 a liga tem capacidade de dobragem limitada e a conforma\u00e7\u00e3o a frio \u00e9 restringida pelo n\u00edvel de resist\u00eancia; formas complexas que se conformam facilmente em T4 fissurar\u00e3o em T6. Confirme os raios de dobragem m\u00ednimos em fun\u00e7\u00e3o da espessura e do temper reais antes de comprometer o ferramental.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Soldagem<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">O 6013 solda bem. Os dados dos produtores de alum\u00ednio classificam a sua soldabilidade no topo da escala e descrevem-no como facilmente un\u00edvel por m\u00e9todos convencionais de soldadura e brasagem \u2014 esta \u00e9 uma das principais vantagens da liga sobre o 2024, que n\u00e3o \u00e9 considerado sold\u00e1vel por fus\u00e3o.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A ressalva habitual continua a aplicar-se: uma soldadura em 6xxx perde resist\u00eancia localmente porque o calor da soldadura sobre-envelhece ou re-solubiliza a estrutura de precipitados na zona de soldadura e nas suas proximidades. Projete para a condi\u00e7\u00e3o como soldado e coloque as soldaduras afastadas dos locais de tens\u00e3o m\u00e1xima sempre que poss\u00edvel. A sele\u00e7\u00e3o do material de adi\u00e7\u00e3o deve seguir os requisitos da junta e qualquer qualifica\u00e7\u00e3o de procedimento aplic\u00e1vel \u2014 consulte o nosso <a href=\"https:\/\/premiumalu.com\/pt\/dicas-de-especialistas-sobre-arame-de-soldagem-de-aluminio-para-o-sucesso\/\">guia de sele\u00e7\u00e3o de fio de soldadura de alum\u00ednio<\/a> para saber como a escolha do material de adi\u00e7\u00e3o interage com a liga base e o ambiente de servi\u00e7o.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Usinagem<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">A maquinabilidade \u00e9 boa, classificada em cerca de 70 na escala padr\u00e3o de 0\u2013100, onde as ligas de corte f\u00e1cil se situam perto de 90. O T651 \u00e9 geralmente preferido para placa fortemente maquinada devido ao al\u00edvio de tens\u00f5es.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Tratamento superficial<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">O 6013 aceita bem a anodiza\u00e7\u00e3o e a pintura. N\u00e3o \u00e9 uma liga decorativa de anodiza\u00e7\u00e3o brilhante \u2014 se o requisito for guarni\u00e7\u00e3o brilhante de apar\u00eancia cr\u00edtica, o 5005, o 5657 ou o 6063 s\u00e3o as respostas padr\u00e3o. Para anodiza\u00e7\u00e3o protetora e pr\u00e9-tratamento de pintura, o 6013 comporta-se sem manuseamento especial.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Limites de corros\u00e3o e temperatura<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A formula\u00e7\u00e3o honesta \u00e9 esta: o 6013 tem <strong>boa<\/strong> resist\u00eancia \u00e0 corros\u00e3o para uma liga contendo cobre, e <strong>menos<\/strong> resist\u00eancia geral \u00e0 corros\u00e3o inferior \u00e0 do 6061. Compara\u00e7\u00f5es publicadas observam uma maior tend\u00eancia \u00e0 corros\u00e3o intergranular no 6013 do que no 6061, particularmente quando o processamento n\u00e3o \u00e9 devidamente controlado \u2014 com efeitos secund\u00e1rios relatados sobre a resist\u00eancia \u00e0 fadiga, ductilidade e resist\u00eancia mec\u00e2nica se n\u00e3o for controlado.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A resist\u00eancia \u00e0 fissura\u00e7\u00e3o por corros\u00e3o sob tens\u00e3o \u00e9 classificada no topo da escala do produtor, o que representa uma melhoria genu\u00edna em rela\u00e7\u00e3o \u00e0s ligas 2xxx com as quais o 6013 compete. Mas o 6013 n\u00e3o \u00e9 uma liga marinha. Para servi\u00e7o em \u00e1gua salgada imerso ou na zona de salpicos, as classes 5xxx continuam a ser a fam\u00edlia correta \u2014 consulte o nosso <a href=\"https:\/\/premiumalu.com\/pt\/marine-grade-aluminum\/\">guia de sele\u00e7\u00e3o de alum\u00ednio de qualidade marinha<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Em rela\u00e7\u00e3o \u00e0 temperatura, o limite pr\u00e1tico \u00e9 de cerca de 160 \u00b0C. As ligas endurecidas por precipita\u00e7\u00e3o perdem resist\u00eancia \u00e0 medida que a temperatura aumenta, e o 6013 n\u00e3o \u00e9 um material para temperaturas elevadas, apesar das suposi\u00e7\u00f5es comuns sobre ligas aeroespaciais.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Onde o 6013 \u00c9 Utilizado<\/h2>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" width=\"800\" height=\"600\" src=\"https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Applications-GoNo-Go.png\" alt=\"\" class=\"wp-image-10626\" srcset=\"https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Applications-GoNo-Go.png 800w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Applications-GoNo-Go-300x225.png 300w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Applications-GoNo-Go-768x576.png 768w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Applications-GoNo-Go-16x12.png 16w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/Applications-GoNo-Go-600x450.png 600w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">As listagens de aplica\u00e7\u00f5es do produtor para o 6013 incluem componentes hidr\u00e1ulicos, corpos de v\u00e1lvulas, pe\u00e7as de m\u00e1quinas, componentes de sistemas de travagem ABS e muni\u00e7\u00f5es. Para al\u00e9m destes, as duas aplica\u00e7\u00f5es de volume s\u00e3o:<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li><strong>Aeroespacial<\/strong> \u2014 revestimentos de aeronaves e pain\u00e9is estruturais, onde a liga \u00e9 avaliada como candidata a substituir a chapa 2024, particularmente onde o comportamento de soldadura ou de corros\u00e3o exclui o 2024.<\/li>\n\n\n\n<li><strong>Automotivo e transporte<\/strong> \u2014 pain\u00e9is estruturais e de carro\u00e7aria, e quadros de bicicletas, guiadores e componentes de rodas, onde \u00e9 necess\u00e1ria resist\u00eancia superior \u00e0 do 6061 numa liga sold\u00e1vel.<\/li>\n<\/ul>\n\n\n\n<h2 class=\"wp-block-heading\">6013 vs. 6061 vs. 2024 vs. 7075<\/h2>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"800\" height=\"600\" src=\"https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-vs-6061-vs-2024.png\" alt=\"\" class=\"wp-image-10625\" srcset=\"https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-vs-6061-vs-2024.png 800w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-vs-6061-vs-2024-300x225.png 300w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-vs-6061-vs-2024-768x576.png 768w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-vs-6061-vs-2024-16x12.png 16w, https:\/\/premiumalu.com\/wp-content\/uploads\/2025\/05\/6013-vs-6061-vs-2024-600x450.png 600w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/figure>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td>Liga met\u00e1lica<\/td><td>Elementos de liga principais<\/td><td>Resist\u00eancia \u00e0 tra\u00e7\u00e3o (MPa)<\/td><td>Corros\u00e3o geral<\/td><td>Soldabilidade<\/td><td>Adequado quando<\/td><\/tr><tr><td><a href=\"https:\/\/premiumalu.com\/pt\/produto\/liga-de-aluminio-6013\/\" data-type=\"product\" data-id=\"2948\">6013-T6<\/a><\/td><td>Mg-Si-Cu<\/td><td>379 \u2013 410<\/td><td>Boa (maior tend\u00eancia \u00e0 CIG do que o 6061)<\/td><td>Bom<\/td><td>Resist\u00eancia da classe 2024 numa pe\u00e7a sold\u00e1vel<\/td><\/tr><tr><td><a href=\"https:\/\/premiumalu.com\/pt\/produto\/liga-de-aluminio-6061\/\" data-type=\"link\" data-id=\"https:\/\/premiumalu.com\/product\/6061-aluminum-alloy\/\">6061-T6<\/a><\/td><td>Mg-Si<\/td><td>240 \u2013 310<\/td><td>Muito boa<\/td><td>Excelente<\/td><td>Trabalho estrutural geral, melhor disponibilidade global<\/td><\/tr><tr><td><a href=\"http:\/\/premiumalu.com\/pt\/produto\/liga-de-aluminio-2024\/\" data-type=\"link\" data-id=\"http:\/\/premiumalu.com\/product\/2024-aluminum-alloy\/\">2024-T3<\/a><\/td><td>Cu-Mg<\/td><td>400 \u2013 480<\/td><td>Ruim<\/td><td>N\u00e3o sold\u00e1vel por fus\u00e3o<\/td><td>Resist\u00eancia m\u00e1xima da classe 2xxx onde a soldadura n\u00e3o \u00e9 necess\u00e1ria<\/td><\/tr><tr><td><a href=\"http:\/\/premiumalu.com\/pt\/produto\/liga-de-aluminio-7075\/\" data-type=\"link\" data-id=\"http:\/\/premiumalu.com\/product\/7075-aluminum-alloy\/\">7075-T6<\/a><\/td><td>Zn-Mg-Cu<\/td><td>500 \u2013 570<\/td><td>Ruim<\/td><td>Ruim<\/td><td>Resist\u00eancia m\u00e1xima, corros\u00e3o e soldadura n\u00e3o s\u00e3o fatores determinantes<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">As duas compara\u00e7\u00f5es que decidem a maioria dos trabalhos:<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>6013 vs 6061.<\/strong> O 6013 \u00e9 significativamente mais resistente. O 6061 \u00e9 mais tolerante \u00e0 corros\u00e3o, mais barato e dispon\u00edvel em todo o lado. Escolha o 6013 quando a margem de resist\u00eancia \u00e9 o que faz falhar o projeto, n\u00e3o como uma atualiza\u00e7\u00e3o padr\u00e3o. Se a resist\u00eancia \u00e0 corros\u00e3o for a prioridade, o 6061 \u00e9 a melhor resposta \u2014 consulte o nosso <a href=\"https:\/\/premiumalu.com\/pt\/guia-completo-do-aluminio-6061\/\">guia completo do alum\u00ednio 6061<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>6013 vs 2024.<\/strong> A resist\u00eancia, tenacidade \u00e0 fratura e fadiga no 6013-T6 aproximam-se das da chapa 2024-T3, com melhor resist\u00eancia \u00e0 corros\u00e3o e menor densidade. O fator decisivo \u00e9 geralmente a liga\u00e7\u00e3o: se a montagem \u00e9 soldada, o 6013 vence; se \u00e9 rebitada e a corros\u00e3o \u00e9 gerida por clad ou acabamento, o 2024 pode ainda ser especificado.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Go \/ No-Go<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Go \u2014 especifique 6013 quando:<\/strong><\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li>\u00c9 necess\u00e1ria uma junta soldada numa pe\u00e7a que requer resist\u00eancia superior \u00e0 do 6061. Pe\u00e7as t\u00edpicas: conjuntos aeroespaciais soldados, manifolds hidr\u00e1ulicos, suportes estruturais.<\/li>\n\n\n\n<li>A pe\u00e7a pode ser conformada em T4 e envelhecida diretamente para T6, evitando um tratamento de re-solu\u00e7\u00e3o. Pe\u00e7as t\u00edpicas: pain\u00e9is de grandes dimens\u00f5es sens\u00edveis \u00e0 distor\u00e7\u00e3o, perfis estruturais estirados.<\/li>\n\n\n\n<li>A resist\u00eancia \u00e0 fadiga \u00e9 um fator de projeto e a resist\u00eancia \u00e0 fadiga do T6 de ~140 MPa cumpre o ciclo de servi\u00e7o. Pe\u00e7as t\u00edpicas: suportes com carregamento din\u00e2mico, estruturas de transporte.<\/li>\n\n\n\n<li>S\u00e3o necess\u00e1rias propriedades da classe 2024-T3, mas o ambiente de servi\u00e7o exclui uma liga 2xxx nua.<\/li>\n\n\n\n<li>Chapa fortemente maquinada onde a estabilidade dimensional \u00e9 importante \u2014 especifique T651.<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>No-Go \u2014 procure alternativas quando:<\/strong><\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li>A resist\u00eancia m\u00e1xima \u00e0 corros\u00e3o \u00e9 a prioridade. O 6061 ou uma liga 5xxx ter\u00e3o melhor desempenho do que o 6013; o teor de cobre joga contra.<\/li>\n\n\n\n<li>A pe\u00e7a opera continuamente acima de aproximadamente 160 \u00b0C.<\/li>\n\n\n\n<li>A exposi\u00e7\u00e3o principal \u00e9 \u00e1gua salgada imersa ou na zona de salpicos. Utilize 5083 ou 5086 \u2014 comece pelo nosso <a href=\"https:\/\/premiumalu.com\/pt\/guia-do-especialista-em-ligas-de-aluminio-5083\/\">guia do alum\u00ednio 5083<\/a>.<\/li>\n\n\n\n<li>\u00c9 genuinamente necess\u00e1ria resist\u00eancia da classe 7075, e a soldadura e a corros\u00e3o n\u00e3o s\u00e3o restri\u00e7\u00f5es vinculativas.<\/li>\n\n\n\n<li>S\u00e3o necess\u00e1rios raios de curvatura apertados na condi\u00e7\u00e3o de entrega. Conforme em T4 e envelhe\u00e7a, ou escolha uma liga mais conform\u00e1vel.<\/li>\n\n\n\n<li>A disponibilidade e o custo dominam. O 6061 est\u00e1 armazenado muito mais amplamente e \u00e9 a op\u00e7\u00e3o padr\u00e3o mais segura.<\/li>\n<\/ul>\n\n\n\n<h2 class=\"wp-block-heading\">Verifica\u00e7\u00f5es de Fornecimento<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O 6013 n\u00e3o \u00e9 uma qualidade de commodity, pelo que o pedido necessita de mais defini\u00e7\u00e3o do que uma linha de encomenda de 6061. Antes de emitir uma ordem de compra, confirme:<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li><strong>Especifica\u00e7\u00e3o e temper juntos<\/strong> \u2014 ASTM B209 ou a designa\u00e7\u00e3o AMS aplic\u00e1vel para chapa (4216 para T6, 4347 para T4), mais o temper. 6013-T6 e 6013-T651 n\u00e3o s\u00e3o intercambi\u00e1veis num desenho.<\/li>\n\n\n\n<li><strong>Faixa de espessura<\/strong> \u2014 os m\u00ednimos mec\u00e2nicos garantidos variam com a espessura. Indique o intervalo que aceita.<\/li>\n\n\n\n<li><strong>Rota de tratamento t\u00e9rmico<\/strong> \u2014 se pretende conformar em T4 e envelhecer para T6, indique-o na fase de encomenda para que o material seja fornecido numa condi\u00e7\u00e3o que o suporte.<\/li>\n\n\n\n<li><strong>\u00c2mbito do MTC<\/strong> \u2014 solicite o certificado com resultados qu\u00edmicos e mec\u00e2nicos, e confirme que o temper e a especifica\u00e7\u00e3o constam do mesmo.<\/li>\n\n\n\n<li><strong>Testes de terceiros<\/strong> \u2014 quando a aplica\u00e7\u00e3o \u00e9 aeroespacial ou pressurizada, acorde o \u00e2mbito de ensaio adicional antecipadamente em vez de o fazer ap\u00f3s a produ\u00e7\u00e3o.<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\">A Linsy Aluminium fornece 6013 em chapa e placa, e apoia maquinagem CNC, soldadura TIG e MIG, corte laser e acabamento superficial internamente, para que o material e o processamento de primeira fase possam ser tratados numa s\u00f3 encomenda. Consulte a <a href=\"https:\/\/premiumalu.com\/pt\/produto\/liga-de-aluminio-6013\/\">liga de alum\u00ednio 6013<\/a> p\u00e1gina de produto para tempers e dimens\u00f5es dispon\u00edveis.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Conclus\u00e3o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O 6013 justifica o seu lugar quando uma pe\u00e7a soldada e sujeita a fadiga necessita de mais resist\u00eancia do que o 6061 proporciona, e quando a conforma\u00e7\u00e3o em T4 e o envelhecimento direto para T6 \u2014 sem novo tratamento de solubiliza\u00e7\u00e3o, sem t\u00eampera adicional \u2014 vale o pr\u00e9mio. O compromisso \u00e9 a disponibilidade: o cobre aumenta a tend\u00eancia \u00e0 corros\u00e3o intergranular em rela\u00e7\u00e3o ao 6061, a liga custa mais, e a maioria dos fabricantes mant\u00e9m muito menos stock do que de 6061 ou 2024.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fornecemos chapa e placa de 6013 segundo as especifica\u00e7\u00f5es padr\u00e3o e realizamos produ\u00e7\u00e3o personalizada de baixo MOQ para tempers e dimens\u00f5es fora destas, com um prazo de entrega de 10 a 60 dias em linhas personalizadas. Cada encomenda \u00e9 expedida com um MTC.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"https:\/\/premiumalu.com\/pt\/contato\/\" data-type=\"link\" data-id=\"https:\/\/premiumalu.com\/contact\/\">Envie-nos o desenho<\/a>, requisitos de temper e espessura para uma an\u00e1lise t\u00e9cnica e or\u00e7amento.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Perguntas frequentes<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Em que formas est\u00e1 dispon\u00edvel o 6013?<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Chapa, placa e bobina s\u00e3o as formas laminadas. Tubo, barra e perfis n\u00e3o padronizados s\u00e3o produzidos segundo o seu desenho, pelo que a liga n\u00e3o se limita a produto plano. Indique o temper juntamente com a forma, porque nem todos os tempers s\u00e3o produzidos em todos os produtos.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Que consum\u00edvel de soldadura devo usar para soldar 6013?<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">ER4043 (AlSi5) ou ER5356 (AlMg5Cr) segundo AWS A5.10. O ER4043 \u00e9 a primeira escolha habitual em metal base 6xxx porque o seu teor mais elevado de sil\u00edcio reduz a sensibilidade \u00e0 fissura\u00e7\u00e3o a quente. Passe para ER5356 quando a junta necessitar de um dep\u00f3sito soldado mais resistente.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Como se compara o 6013 com o 6061 em custo e disponibilidade?<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Custa mais e \u00e9 armazenado com muito menos amplitude. O 6061 \u00e9 uma liga de grande consumo mantida pela maioria dos centros de servi\u00e7o, enquanto o 6013 \u00e9 uma liga de nicho aeroespacial, pelo que o prazo de entrega depende de o seu temper e espessura estarem em stock ou serem produzidos. Preveja o pr\u00e9mio e confirme a disponibilidade antes de se comprometer com uma data de entrega.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>O 6013 pode ser cortado ou maquinado segundo desenho antes da expedi\u00e7\u00e3o?<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Sim. Corte \u00e0 medida, maquinagem CNC, corte laser e quinagem s\u00e3o realizados internamente, pelo que as pe\u00e7as podem chegar pr\u00f3ximas da dimens\u00e3o final. Envie o desenho com o seu pedido e as toler\u00e2ncias e especifica\u00e7\u00f5es de superf\u00edcie s\u00e3o or\u00e7amentadas juntamente com o material.<\/p>","protected":false},"excerpt":{"rendered":"<p>6013 exists for one design problem: a part that needs 2024-T3-class strength but has to be welded. 6061 will weld, but it runs out of strength just above 310 MPa in T6. 2024-T3 has the strength, but it is not a fusion-welding alloy and needs cladding or paint to survive service. 6013 closes that problem [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":10624,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_seopress_titles_title":"6013 Aluminum: Properties, Tempers, and When to Specify","_seopress_titles_desc":"Specifying 6013 aluminum? See composition, T4\/T6\/T651 mechanical properties, the form-then-age route, and welding and corrosion limits vs 6061 and 2024.","_seopress_robots_index":"","_seopress_robots_follow":"","_seopress_robots_imageindex":"","_seopress_robots_snippet":"","_seopress_robots_primary_cat":"","_seopress_robots_breadcrumbs":"","_seopress_robots_freeze_modified_date":"","_seopress_robots_custom_modified_date":"","_seopress_robots_canonical":"","_seopress_social_fb_title":"","_seopress_social_fb_desc":"","_seopress_social_fb_img":"","_seopress_social_fb_img_attachment_id":0,"_seopress_social_fb_img_width":0,"_seopress_social_fb_img_height":0,"_seopress_social_twitter_title":"","_seopress_social_twitter_desc":"","_seopress_social_twitter_img":"","_seopress_social_twitter_img_attachment_id":0,"_seopress_social_twitter_img_width":0,"_seopress_social_twitter_img_height":0,"_seopress_redirections_value":"","_seopress_redirections_enabled":"","_seopress_redirections_enabled_regex":"","_seopress_redirections_logged_status":"","_seopress_redirections_param":"","_seopress_redirections_type":0,"_seopress_analysis_target_kw":"","footnotes":""},"categories":[177],"tags":[],"class_list":["post-8721","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-5000_6000-series-aluminum"],"_links":{"self":[{"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/posts\/8721","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/comments?post=8721"}],"version-history":[{"count":2,"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/posts\/8721\/revisions"}],"predecessor-version":[{"id":10628,"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/posts\/8721\/revisions\/10628"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/media\/10624"}],"wp:attachment":[{"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/media?parent=8721"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/categories?post=8721"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/premiumalu.com\/pt\/wp-json\/wp\/v2\/tags?post=8721"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}